Abstract:Using PhBr and BF3: OEt2 as the raw materials, the poly(p-phenylene borane) (PPB) is synthesized, After PPB is pyrolyzed in high temperature, the product containing 54.4% B4C. 32% free canbon and 13.6% B2O3 is obtained. If the carbon fiber(Cf) is dipped in the solution of PPB and pyrolyzed in high temperature, the Cf coated by B4C (B4C-Cf) is obtained, Comparing with raw Cf in same treat conditions, the tempereture of thermal oxidation resistance of B4C-Cf has increased by 200℃. The δ6 of Cf/SiC matrix composites made by using B4C-Cf 1800℃ is improved 10.5% and the KIC is improved 19.4%. At 1850℃, the δь is improved 31.6% and the KIC is improved 5.8%.